Paper
Platinized Titanium as Alternative Cost‐Effective Anode for Efficient Kolbe Electrolysis in Aqueous Electrolyte Solutions
Summary
What the paper reports, in its own words.
Abstract
Five commercial materials were assessed for electrochemical conversion of n ‐hexanoic acid by Kolbe electrolysis. Platinized titanium performed best, achieving a coulombic efficiency (CE) of 93.1±6.7 % ( n =6) for the degradation of n ‐hexanoic acid and 48.3±3.2 % ( n =6) for the production of n ‐decane, which is close to the performance of pure platinum (89.7±14.4 and 55.5±3.5 %; n =6). 56.7 mL liquid fuel was produced per mole n ‐hexanoic acid, converting to an energy demand of 6.66 kWh and 1.22 € per L. Using optical profilometry and scanning electron microscopy coupled with energy‐dispersive X‐ray spectroscopy, it was shown that the degree of coverage of the titanium surface with platinum played the most important role. An uncovered surface of as little as 1–3 % already led to a deterioration of the CE of approximately 50 %. Using platinized titanium requires >36 times less capital expenditure at only <10 % increased operational expenditure; an electrode lifetime of 10000 h can be expected.
Extracted values
Every value pulled from the paper, with its source, so each number can be checked against the text.
n = 61 extracted values
Select a citation to see the quote, page and confidence behind a value.
0 of 61 extracted rows modelable
- 61 not canonicalised (no canonical slug)
| Parameter | Value | Unit | Confidence | Source | Notes | Modelable |
|---|---|---|---|---|---|---|
| Working volume of anode chamber | 200 | mL | 100% | extracted | "The working volume of the anode chamber was 200 mL and that of the cathode chamb…" · cell=two-chamber, fumasep FKS-PET-130 ion exchange membrane | Excluded: not canonicalised (no canonical slug) |
| Distance between working and counter electrode | 18 | mm | 100% | extracted | "keeping the WE and the CE chamber in a defined position with a 18 mm distance be…" · cell=electrode holder, three-neck 250 mL flask | Excluded: not canonicalised (no canonical slug) |
| Working volume of cathode chamber | 9 | mL | 100% | extracted | "The working volume of the anode chamber was 200 mL and that of the cathode chamb…" · cell=two-chamber, fumasep FKS-PET-130 ion exchange membrane | Excluded: not canonicalised (no canonical slug) |
| Working electrode geometric surface area | 2 | cm² | 100% | extracted | "a WE with a geometric surface area of 2 cm2" · electrode=working electrode (WE) | Excluded: not canonicalised (no canonical slug) |
| Total charge passed (Qtotal) | 4,320 | C | 100% | extracted | "Since all experiments were carried out galvanostatically, Qtotal was always 4320…" · cell=two-chamber, time=4 h, acids=["n-hexanoic acid"], electrolyte=0.25 m Na2SO4, pH 7 | Excluded: not canonicalised (no canonical slug) |
| Charge transferred per experiment | 0.44 | Faraday equivalents | 100% | extracted | "Since all experiments were carried out galvanostatically, Qtotal was always 4320…" · cell=two-chamber, time=4 h, acids=["n-hexanoic acid"], electrolyte=0.25 m Na2SO4, pH 7 | Excluded: not canonicalised (no canonical slug) |
| Na2SO4 supporting electrolyte concentration | 0.25 | mol L⁻¹ | 100% | extracted | "The conductivity was adjusted by adding Na2SO4 to a concentration of 0.25 mol L-…" · acids=["n-hexanoic acid"], cation=Na+ | Excluded: not canonicalised (no canonical slug) |
| Initial pH of reaction solution | 7 | — | 100% | extracted | "the pH of the solution was adjusted to pH=7 using NaOH pellets and H2SO4" · acids=["n-hexanoic acid"], electrolyte=0.25 mol L−1 Na2SO4 | Excluded: not canonicalised (no canonical slug) |
| Constant current applied | 300 | mA | 100% | extracted | "The electrolysis was carried out for 4 h with a constant current of 300 mA at ro…" · cell=two-chamber, time=4 h, acids=["n-hexanoic acid"], electrolyte=0.25 m Na2SO4, pH 7 | Excluded: not canonicalised (no canonical slug) |
| Current density (galvanostatic), electrode screening | 150 | mA cm⁻² | 100% | extracted | "Overview of different anode materials for Kolbe electrolysis of n-hexanoic acid …" · cell=two-chamber, time=4 h, acids=["n-hexanoic acid"], electrolyte=0.25 m Na2SO4, pH 7 | Excluded: not canonicalised (no canonical slug) |
| Electrolysis time | 4 | h | 100% | extracted | "The electrolysis was carried out for 4 h with a constant current of 300 mA at ro…" · cell=two-chamber, time=4 h, acids=["n-hexanoic acid"], electrolyte=0.25 m Na2SO4, pH 7 | Excluded: not canonicalised (no canonical slug) |
| Stirring speed of anode chamber solution | 1,000 | rpm | 100% | extracted | "The electrolysis was carried out for 4 h with a constant current of 300 mA at ro…" · cell=two-chamber, time=4 h, acids=["n-hexanoic acid"], electrolyte=0.25 m Na2SO4, pH 7 | Excluded: not canonicalised (no canonical slug) |
| n-decane yield per n-hexanoic acid (Y decane), platinized Ti Type B | 52.3 ±6.9 | % | 95% | extracted | "platinized Ti Type B (n=6) | 65.0±7.5 | 52.3±6.9 | 66.9±0.9" · cell=two-chamber, time=4 h, acids=["n-hexanoic acid"], electrode=platinized Ti Type B | Excluded: not canonicalised (no canonical slug) |
| Selectivity for n-decane production (S decane), platinized Ti Type A | 63.9 ±2.3 | % | 95% | extracted | "platinized Ti Type A (n=3) | 77.2±51.4 | 60.4±43.0 | 63.9±2.3" · cell=two-chamber, time=4 h, acids=["n-hexanoic acid"], electrode=platinized Ti Type A | Excluded: not canonicalised (no canonical slug) |
| Selectivity for n-decane production (S decane), Pt/Ir on Ti | 49.9 ±17.5 | % | 95% | extracted | "Pt/Ir on Ti (n=3) | 31.2±67.6 | 21.2±52.6 | 49.9±17.5" · cell=two-chamber, time=4 h, acids=["n-hexanoic acid"], electrode=Pt/Ir on Ti | Excluded: not canonicalised (no canonical slug) |
| n-decane yield per n-hexanoic acid (Y decane), Pt/Ir on Ti | 21.2 ±52.6 | % | 95% | extracted | "Pt/Ir on Ti (n=3) | 31.2±67.6 | 21.2±52.6 | 49.9±17.5" · cell=two-chamber, time=4 h, acids=["n-hexanoic acid"], electrode=Pt/Ir on Ti | Excluded: not canonicalised (no canonical slug) |
| Selectivity for n-decane production (S decane), platinized Ti Type B | 66.9 ±0.9 | % | 95% | extracted | "platinized Ti Type B (n=6) | 65.0±7.5 | 52.3±6.9 | 66.9±0.9" · cell=two-chamber, time=4 h, acids=["n-hexanoic acid"], electrode=platinized Ti Type B | Excluded: not canonicalised (no canonical slug) |
| Pt concentration in aqueous phase after electrolysis (cPt), pure Pt | 24.6 ±9.47 | ng mL⁻¹ | 95% | icp-ms | "pure Pt (n=3) | 24.63±9.47" · cell=two-chamber, time=4 h, acids=["n-hexanoic acid"], electrode=pure Pt foil | Excluded: not canonicalised (no canonical slug) |
| Pt concentration in aqueous phase after electrolysis (cPt), platinized Ti Type A | 99 ±10.03 | ng mL⁻¹ | 95% | icp-ms | "platinized Ti Type A (n=3) | 99.00±10.03" · cell=two-chamber, time=4 h, acids=["n-hexanoic acid"], electrode=platinized Ti Type A | Excluded: not canonicalised (no canonical slug) |
| Pt concentration in aqueous phase after electrolysis (cPt), platinized Ti Type B | 25.9 ±3.83 | ng mL⁻¹ | 95% | icp-ms | "platinized Ti Type B (n=6) | 25.85±3.83" · cell=two-chamber, time=4 h, acids=["n-hexanoic acid"], electrode=platinized Ti Type B | Excluded: not canonicalised (no canonical slug) |
| n-decane yield per n-hexanoic acid (Y decane), platinized Ti Type A | 60.4 ±43.0 | % | 95% | extracted | "platinized Ti Type A (n=3) | 77.2±51.4 | 60.4±43.0 | 63.9±2.3" · cell=two-chamber, time=4 h, acids=["n-hexanoic acid"], electrode=platinized Ti Type A | Excluded: not canonicalised (no canonical slug) |
| Coulombic efficiency for n-hexanoic acid degradation (CE hexanoic acid) | 93.1 ±6.7 | % | 95% | extracted | "Platinized titanium performed best, achieving a coulombic efficiency (CE) of 93.…" · cell=two-chamber, time=4 h, acids=["n-hexanoic acid"], electrode=platinized Ti Type B | Excluded: not canonicalised (no canonical slug) |
| Coulombic efficiency for n-decane (CE decane) | 48.3 ±3.2 | % | 95% | extracted | "Platinized titanium performed best, achieving a coulombic efficiency (CE) of 93.…" · cell=two-chamber, time=4 h, acids=["n-hexanoic acid"], electrode=platinized Ti Type B | Excluded: not canonicalised (no canonical slug) |
| Coulombic efficiency for n-hexanoic acid degradation, one-chamber cell | 94.1 ±17.4 | % | 95% | extracted | "This was confirmed for both one- and two-chamber setups, with a CEhexanoic acid …" · cell=one-chamber, time=4 h, acids=["n-hexanoic acid"], electrode=pure Pt foil | Excluded: not canonicalised (no canonical slug) |
| Coulombic efficiency for n-hexanoic acid degradation, two-chamber cell | 89.7 ±14.4 | % | 95% | extracted | "This was confirmed for both one- and two-chamber setups, with a CEhexanoic acid …" · cell=two-chamber, time=4 h, acids=["n-hexanoic acid"], electrode=pure Pt foil | Excluded: not canonicalised (no canonical slug) |
Pipeline
Raw extractions, artifacts, quality signal
Extraction quality
honesty signalCalibrate your trust in the extracted content against these signals — they're how the pipeline rated its own output for this paper.
Mean parameter confidence
92%
Average confidence across PaperParameter rows surfaced above
review against source PDF before citing · scores 0–1
Chart explorer
Move the inputs this paper used and see how the predicted outcome shifts.
Explore model
The reactor in 3D, with flow you can switch on and off.
AI insights
Contradictions, gaps and opportunities found by comparing this paper with the corpus.
Compare similar papers
The nearest papers by system, materials and organisms, with their outcomes side by side.
Source PDF
The paper as published.
No 3D model is mapped to this paper yet. The values extracted from it are listed under Extracted values.
Keywords
- Kolbe electrolysis
- Coulombic efficiency
- anode materials
- electrode lifetime
- aqueous electrolyte solutions
- cost-effectiveness
- liquid fuel production
Cite
Katharina Neubert, Matthias Schmidt, Falk Harnisch (2021). Platinized Titanium as Alternative Cost‐Effective Anode for Efficient Kolbe Electrolysis in Aqueous Electrolyte Solutions. ChemSusChem. https://doi.org/10.1002/cssc.202100854
- Journal
- ChemSusChem